EN 10025-2 Standard

W.NR.: 1.0044/S275JR

Non-Alloy Steel for Structural Purposes

Heat analysis according to the EN 10025-2 standard

C %Si %Mn %P %S %N %Cu %
for thicknesses in mm
 ≤16       >16 ≤40       >40
From
To0,210,210,221,500,0350,0350,0120,55

According to the UNI 10233-3 standard

Thickness mmCold Drawn
( +C )
Rp0,2  minimumRm minimumA5 %
(MPa)(MPa)minimum
≤5490590 ÷ 8806
>5≤10440540 ÷ 8407
>10≤16380540 ÷ 8407
>16≤25340540 ÷ 7658
>25≤40300490 ÷ 7359
>40≤80265440 ÷ 70011
>80

* Delivery condition: as rolled.

Weldability:
This steel grade is generally suitable to welding.

Notes:

CORRESPONDENCE WITH OTHER STANDARDS (purely as an indication):

EN 10025-2:04EN 10025:90UNI 7070DIN 17 100NF A35-501
 S275JR Fe 430 B Fe 430 B St 44-2 E 28-2